AZ50XT single coat
Robert Black
I've used the lower viscosity AZ40XT to coat and pattern 40um with good
results. I used the vendor recommendations except for a 30 sec longer PEB
(2nd one).
Here are the bake temps/times.
Time Temp
Coat
Soft bake1 120S 100C
Soft bake2 120S 110C
Soft bake3 180S 125C
Expose
PEB1 20S 100C
PEB2 120S 105C vendor recommended 90S
Develop 4 puddles
This resist is chemically amplified so I think the 105 temp is fairly
critical.
Robert
-----Original Message-----
From: mems-talk-bounces@memsnet.org [mailto:mems-talk-bounces@memsnet.org]
On Behalf Of Haixin Zhu
Sent: Tuesday, November 18, 2008 5:26 PM
To: General MEMS discussion
Subject: [mems-talk] AZ50XT single coat
Dear all,
I am trying to have 60um thick AZ 50XT on top of quartz substrate, and
having some issues with the pattern undercut and film stress, is there
anyone who can provide a working recipe since the protocol from the
vendor seems not working well.
Appreciate the help